Hello Folks
Is there any way that I could determine weather or not I would be able to reach Almen "A" .018-.022 with CCW14 with 13" wheel @ 3600 rpm?
With a little bit of math that was exactly what I needed Thanks Jack
My maths indicates that you will have just over 200 feet per second of shot speed. That would require S280 to S230 using Jack's chart. That is much larger than CCW14. My conclusion is that you would not be able to achieve the required intensity. Do you agree?
Even if you could achieve the desired intensity, I would advise you don’t do it. Peening at that high of velocity is not peening its blasting. You will be abusing the surface of the part in my opinion.
Thanks for the Info Folks I have taken it all into consideration.
Is there anything similar to this for up to 780?