Abstract:
Shot peening improves fatigue resistance mainly by introducing self stresses (residual stresses). The compressive self stresses near the surface are balanced by tensile
self stresses which decrease fatigue strength in the interior where stresses are usually lower.
T
he magnitude and distribution of the peening stresses depend mainly on the materials, not on the intensity. The intensity (specified in Almen numbers) determines the depth
to which the compressive stresses extend below the peened surface. A low peening intensity will not increase the fatigue resistance as much as a higher intensity. Very
high peening intensities may not increase the fatigue resistance as much as a lower intensity, partly because the tensile stresses at the interior become too high and partly
because the compressive stresses become less for great depth of peening than for shallow peening. The optimum intensity is defined by the depth at which both decreased
intensity and increased intensity would decrease the fatigue resistance. Figure 1 gives an example of optimum depth, based on assumptions explained in the discussion.