AMS 2430 3.4.3.1 All edges and corners in the areas to be peened shall be inspected and be free of sharp edges and burrs.

This is a vague statement in my opinion. I think the specification(s) needs to define what a sharp edge is and provide guidance as to what a minimum edge break should be in APR 7488.

ARP 7488
3.5 Pre-peening Part Considerations 3.5.1 Parts should be provided to the peening processor by the purchaser in a condition prepared and ready for the peening process. The planned sequence of operations should result in parts provided to the processor that are free of grease, dirt, oil, corrosion, burrs, sharp edges, mechanical damage and corrosion-preventive coatings such as anodic coatings, plating, or paint. All burrs should be removed, and edges and corners to be peened should be rounded prior to peening to prevent material rollover. All heat treatment and non-destructive testing should be completed prior to peening. The part should be provided to the processor with all part dimensions and finish requirements met.

Joined: Jan 2019
Posts: 1
Z
ZHU Offline
Member
Offline
Member
Z
Joined: Jan 2019
Posts: 1
have u solve the problem of edge rollover?

Joined: May 1999
Posts: 202
Walter Offline OP
Member
OP Offline
Member
Joined: May 1999
Posts: 202
ZHU,

There is nothing in the specification detailing what the edge break should be yet, unfortunately. The engineering drawing call out for edge break always takes precedence over any specification.

However I have seen an alarming trend whereas the engineering drawing range will not yield and acceptable part after shot peen. Example: UOS all edges are to be broken .003-.015". While an edge broken to .003" would meet drawing requirements, the edge would almost certainly roll at any "A" scale intensity. Whereas if the edge was broken .010-.015" you would just about 100% guarantee that there would be no edge roll. My suggestion for peened parts would be to always put as close to the largest edge break allowed by the drawing. Waiting for this to be addressed by the specification could take years if ever.

Joined: Aug 2022
Posts: 1
P
Member
Offline
Member
P
Joined: Aug 2022
Posts: 1
I think we should make the Peen Specifications clearer when it comes inspecting the edges in areas to be peened, pre and post peen. Initial qualification of the peen process we should be more specific on how we inspect edges in the post peen condition in order to confirm all edges are free from roll over caused by the peening. Also shot Peeners typically preform a general visual inspection before peen, I think peeners should "sharpen" their focus when it comes to the size and quality of all edges to be peened. IF edges are suspect, the part manufacturer should be alerted and should improve their process prior to peening any parts. Edges to be peened should be .010 inches minimum and properly rounded.

For Critical Parts

Qualify Peen process: (Direct and Destructive Inspection)
Inspect edges using white light at 10X-30X magnification or by destructive testing at higher magnification such as 200X-500X.

Production Peening
Inspect part to confirm peen coverage and confirm edge condition Post Peen by using white light and 10X-30X Magnification.