I have a client that want to do a vibro stone tumble operation after shot peening RC 56/58 hardened steel components to an arc hieght of 16/18. I cautioned them that Shot peening should be the last operaton done to a surface, but question what harm such minimal material removal would do. Does any one have an opinion on that ?

Joined: Feb 2006
Posts: 112
S
Member
Offline
Member
S
Joined: Feb 2006
Posts: 112
AMS 2432B gives useful guidelines for the amount of material that can safely be removed post-peening. Briefly: hard materials can have 5% of the Almen A intensity removed and 10% for soft materials. Vobro stone tumbling would be expected to smooth a peened surface - provided that strict control was applied. Without further information it seems that tumbling could be safely applied.

Joined: Nov 2013
Posts: 2
M
Member
OP Offline
Member
M
Joined: Nov 2013
Posts: 2
Hi Thanks for the advise !

Joined: Mar 2014
Posts: 25
A
Member
Offline
Member
A
Joined: Mar 2014
Posts: 25
dear all,

can give some advice about how to measure penning intensity by use almen strip in gear ( helical , worm ..etc )?

wait for reply
thanks
amit89

Joined: May 1999
Posts: 202
Member
Offline
Member
Joined: May 1999
Posts: 202
Amit89,

This is a the single most important part of the shot peening process. I suggest you obtain a copy of SAE J443 go to http://standards.sae.org/j443_201006/ to get yourself a copy. This will help guide you.

Then I think you need to seek out some assistance from someone whom can perform some professional training. This is not a topic that can be easily explained in a internet blog.

Joined: Apr 1999
Posts: 345
Likes: 1
J
Member
Offline
Member
J
Joined: Apr 1999
Posts: 345
Likes: 1
You might be able to benefit from using the new Mini-Strip from Electronics Inc.
http://electronics-inc.com/ministrips.html