we are having problems maintaining consistency with our siphon fed shot peen cabinet.we are interested to know if there are any diagrams or information available on how to set up for maximum consistency.any responses can be emailed to me at [email protected]

thank you

#65 03/03/06 09:31 PM
Joined: Feb 2006
Posts: 112
S
Member
Offline
Member
S
Joined: Feb 2006
Posts: 112
Solution of your problem depends upon the nature of the observed inconsistency. Overall consistency requires constancy of such factors as air pressure, shot quality, velocity, gun-to-component distance, shot impingement angle, shot flow rate, peening time etc.

#66 03/03/06 11:12 PM
Joined: Apr 1999
Posts: 344
Likes: 1
J
Member
Offline
Member
J
Joined: Apr 1999
Posts: 344
Likes: 1
There are many factors to consider when consistency is lacking. I'll list a few of them here:
1. Almen holder flatness
2. Almen strip quality (flatness, hardness)
3. Almen gage calibration
4. Almen gage zero block (flatness)accuracy
5. Air pressure
6. Shot Flow rate (will affect velocity and intensity)
7. Targeting, nozzle alignment
8. Method of determining intensity (implies saturation curve, 4 or more Almen strips, interpretation of 10% rule)

What is it you mean my "consistency"? Please descibe the test you apply and how you perform it.