I'm using Stainless Steel Conditioned Cut Wire Shot.

AMS2430 Table 2B for shape requirements tells me that the max allowable number of unacceptable shapes (For example 47 AWS) is 22.

Whereas AMS2431/4 Table 2 tells me that the max is 2 or .1% of 5 fields viewed for 47 AWS.

Which is it?

Top
#1420 - 05/09/19 11:02 AM Re: Media Shot Shape Requirements [Re: Rich]
Dennis Scharer Offline


Registered: 01/16/07
Posts: 12
Loc: Adrian, Mi
Rich please keep in mind 2430 is an in process specification and 2431/4 is a new material specification. New media will have a tighter specification.