Our customer drawing required shot peening with below shot:
SHOT SIZE 550
INTENSITY 12-14C
COVERAGE 200%
SHOT TYPE NON MAG

Non Mag shot is very new to me. Please help me explain "non mag shot" is made from what material?

Thank you and appreciate your support.

donhan #1323 01/30/18 12:43 PM
Joined: Jan 2007
Posts: 12
D
Member
Offline
Member
D
Joined: Jan 2007
Posts: 12
Donhan

I would suggest going back to your customer and asking them to define the shot requirement. Maybe they could inform you of the media specification. 550 size is normally associated with cast steel shot which is magnetic. There is stainless cut wire, glass and ceramic peening media.

Last edited by Dennis Scharer; 01/30/18 12:44 PM.
donhan #1325 01/31/18 09:42 AM
Joined: Aug 2016
Posts: 15
D
donhan Offline OP
Member
OP Offline
Member
D
Joined: Aug 2016
Posts: 15
Hi Dennis,

Thank you for your reply.

donhan #1523 03/11/21 02:06 AM
Joined: Mar 2021
Posts: 2
W
Member
Offline
Member
W
Joined: Mar 2021
Posts: 2
Hi Donhan,
Non-mag shot should be made of 304 stainless steel, and non mag treatment on this materials.

donhan #1553 10/14/21 01:39 PM
Joined: Mar 2021
Posts: 9
Likes: 1
V
Member
Offline
Member
V
Joined: Mar 2021
Posts: 9
Likes: 1
Hi, Donhan,
You may well have solved this problem but just for the record, you could try using Guysons Spherically Conditioned Stainless Steel Cut Wire Shot. it comes in many sizes, the closest to 550 would probably be made from the Ø1.5mm cut wire.

1 member likes this: Nerigo
Very Old Tom #1555 11/24/21 03:54 PM
Joined: Aug 2021
Posts: 1
N
Member
Offline
Member
N
Joined: Aug 2021
Posts: 1
Hello Tom, thank you for your advice. My teammates have similar project and they were looking for a solution. Tomorrow when I live my house I will stop by at their office and will let them know. Thank once again


Greek residence permit https://tranio.com/greece/residence/
donhan #1556 11/24/21 05:50 PM
Joined: Apr 1999
Posts: 333
J
Member
Online Content
Member
J
Joined: Apr 1999
Posts: 333
Donhan, To be cautious you should ask your customer to be more specific about the non-magnetic shot. It is possible they did not want a metallic shot in order to prevent ferrous contamination or rust. They may have thought they would get ceramic beads or glass beads with their request.


Link Copied to Clipboard
Sponsored by Electronics Inc. © 2022 Electronics Inc. All Rights Reserved.
Powered by UBB.threads™ PHP Forum Software 7.7.5