You state that the material is aluminium but is surely an aluminium alloy. The surface flow characteristics are consistent with an excessive amount of shot (having too high an intensity) being fired at an angle to the component's surface using a wheel-blast machine. A stated "100% coverage" is difficult to either monitor or control. Suggest lowering both peening intensity and coverage together with trying to have shot impact nearer to 90 degrees to the surface.